Fractography by SEM
4 cases · 13 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Brittle Fracture

ML00093 / Sep.2017
MIC of a Drilling Tool
M - Low Alloy Medium Carbon QTP - Heat Treated PartAp - O&G Well DrillingCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Fracture

ML00007 / Dec.2020
Free Machining Brass in Shear Pin
M - BrassP - Machined PartAp - LiftingCd - Shear
Cm - Fractography by SEMDf - Elongated Dimples
More from these cases

ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets

ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Brittle Fracture

ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00093 / Sep.2017
MIC of a Drilling Tool
M - Low Alloy Medium Carbon QTP - Heat Treated PartAp - O&G Well DrillingCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00093 / Sep.2017
MIC of a Drilling Tool
M - Low Alloy Medium Carbon QTP - Heat Treated PartAp - O&G Well DrillingCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00093 / Sep.2017
MIC of a Drilling Tool
M - Low Alloy Medium Carbon QTP - Heat Treated PartAp - O&G Well DrillingCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Ductile Fracture

ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Intergranular Cracking

ML00007 / Dec.2020
Free Machining Brass in Shear Pin
M - BrassP - Machined PartAp - LiftingCd - Shear
Cm - Fractography by SEMDf - Ductile Fracture