Crevice Corrosion in a Subsea System — Aspect Before Analysis

The fracture surface of the main pipe is presented in low magnification (external pipe surface in the top) showing a flat propagation starting from the contour of the weld margin.
173
ML00006 / Apr.2017
Vibration Induced Fatigue in 304SS
M - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Margin of the Weld Crack

More from these cases

ML00006 — Vibration Induced Fatigue in 304SSM - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Fracture surface micromechanism by striation, evidence of FATIGUE.
158
ML00006 / Apr.2017
Vibration Induced Fatigue in 304SS
M - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation
Fracture surface micromechanism by striation, evidence of FATIGUE.
147
ML00006 / Apr.2017
Vibration Induced Fatigue in 304SS
M - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation