Optical Microscope

2 cases · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Optical Microscope — sub-branches

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking
Micrography of the weld metal presenting a martensitic island with microcracks, due to a localized increase in the manganese and silicon content, probably because an active flux was adopted in a condition where a high cleanning action was not required. A high flux-to-wire ratio (>1) could also be an issue.
794
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks

More from these cases

ML00072 — Liquation Cracks in a High Strength JointM - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00067 — Cold Cracks in C-Mn SAW Weld MetalM - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fracture
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks