Structure
1 case · 8 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Condition: Shooting Effect ×Microstructure: Granular ×Capture method: Fractography by SEM ×clear all

ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Dimples
More from these cases

ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Elongated Dimples

ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Elongated Dimples

ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Dimples

ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Elongated Dimples

ML00145 / Sep.2018
Impact of a .380 Winchester on 6061 T6 Plate
M - Aluminum Magnesium SiliconP - Rolled PlateAp - StructureCd - Pierced
Cm - Fractography by SEMDf - Ductile Fracture