Offshore

11 cases · 25 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00016 / Apr.2017
SCC in Free Cutting 303SS
M - Austenitic Stainless SteelP - Machined PartAp - OffshoreCd - Stress Corrosion
Cm - Micrography by OM using A262 Method ADf - Non Metallic Inclusions
ML00036 / Jan.2018
High Strength Medium Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Predominantly Pearlitic
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Banded Structure

More from these cases

ML00036 — High Strength Medium Carbon Steel WireM - Medium Carbon SteelP - WireAp - OffshoreCd - Typical manufacturing
ML00036 / Jan.2018
High Strength Medium Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Typical manufacturing
Cm - Nital Etched Micrography by OMDf - Predominantly Perlitic
ML00013 — Welding Cracks in Mooring ChainM - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Non Metallic Inclusions