Crevice Corrosion in a Subsea System — Aspect Before Analysis

Steam drum presenting cracks in the shell, connecting tube holes.
1704
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Aspect Before AnalysisDf - Cracking

More from these cases

ML00020 — Intergranular SCC in Boiler Steam Drum RepairM - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Aspect of the drum shell after removing the tubes and macroetching, indicating that the cracks were located in repair welded regions.
342
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Aspect by NDTDf - Cracks
A small sample was removed from the steam drum and the micrography shows that the cracks are intergranular (previous austenite) and located in the weld metal.
285
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
The micrography of the small sample removed from the steam drum shows that the cracks are intergranular (previous austenite) and located in the weld metal.
274
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Secondary cracks in the weld metal showing an intergranular morphology. Stress Corrosion Cracking.
249
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking
Detail of the secondary cracks in the weld metal with intergranular morphology. Stress Corrosion Cracking.
251
ML00020 / Apr.2017
Intergranular SCC in Boiler Steam Drum Repair
M - Low Carbon SteelP - Repair WeldAp - BoilerCd - Stress Corrosion
Cm - Nital Etched Micrography by OMDf - Corrosion Cracking

+1 more from this case →