Atlas

3 cases · 11 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
Aspect of the bolt fracture surface by scanning electron microscopy, (SEM) presenting striations that indicate a FATIGUE micromechanism.  The bolt is of a medium strength (class 8.8) low alloy steel, medium carbon, quenched and tempered.
1123
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Fractographic aspect of the broken fastener, at the surface, showing na intergranular morphology typical of a hydrogen assisted mechanism of a high strenght steel under cathodic protection.
224
ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking

More from these cases

ML00136 — Hydrogen Cracks of Subsea StudsM - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks
ML00130 — Fatigue Fracture of Overloaded BoltsM - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Aspect of the fracture surface in low magnification, showing a flat aspect (associated to a fatigue fracture micromechanims) and a rough aspect (associated to a ductile fracture micromechanism).
167
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - General View
Aspect of the fracture surface by scanning electron microscopy, presenting fatigue striations micromechanism.  The bolt is a medium strength low alloy steel, medium carbon, quenched and tempered.
154
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Detailed fractographic aspect of the flat part of the bolt fracture, presenting fatigue striations.  The bolt is a medium strength low alloy steel, medium carbon, quenched and tempered.
141
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
Fractographic detailed aspect of the rough part of the fracture surface, presenting ductile dimples.  This is the final fracture, by overload.
137
ML00130 / Jun.2018
Fatigue Fracture of Overloaded Bolts
M - Low Alloy Medium Carbon QTP - FastenerAp - O&G Well DrillingCd - Mechanical Fatigue
Cm - Fractography by SEMDf - Ductile Fracture
ML00074 — Hydrogen Cracking of a 17-4 PH Subsea BoltM - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Microscopic aspect of the fracture, close to the bolt surface where the fracture is macroscopically brittle, presenting a predominantly intergranular fracture micromechanism.
108
ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Ductile Fracture