Atlas

5 cases · 16 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Detail of the fracture surface, predominantly transgranular with secondary cracks of intergranular morphology.
831
ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Crack
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
The fracture surface of the main pipe is presented in low magnification (external pipe surface in the top) showing a flat propagation starting from the contour of the weld margin.
173
ML00006 / Apr.2017
Vibration Induced Fatigue in 304SS
M - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Margin of the Weld Crack
After opening the crack the fracture surface presented different aspects close to the internal surface and through the wall propagation.  Intergranular at the surface, showing intergranular SCC mechanism, and transgranular with striation, showing the contribution of pulsing loads.
101
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Fractography by SEMDf - Through Wall Cracking

More from these cases

ML00078 — Hydrogen Cracking of IN 718 Subsea ConnectorM - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00012 — Vibration Induced Fatigue in a 316/316L SSM - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Pitting
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Pitting
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation
ML00012 / Aug.2017
Vibration Induced Fatigue in a 316/316L SS
M - Austenitic Stainless SteelP - Seamless PipeAp - OffshoreCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation
ML00041 — Fatigue Fracture of Inconel 718 Spline ShaftM - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Fracture
ML00006 — Vibration Induced Fatigue in 304SSM - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Fracture surface micromechanism by striation, evidence of FATIGUE.
158
ML00006 / Apr.2017
Vibration Induced Fatigue in 304SS
M - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation
Fracture surface micromechanism by striation, evidence of FATIGUE.
147
ML00006 / Apr.2017
Vibration Induced Fatigue in 304SS
M - Austenitic Stainless SteelP - Longitudinal Seam Welded PipeAp - PipingCd - Vibration Induced Fatigue
Cm - Fractography by SEMDf - Fatigue Striation
ML00011 — Intergranular SCC of Pure NickelM - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Fractography by SEMDf - Intergranular Cracking
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Fractography by SEMDf - Fatigue Striation
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Fractography by SEMDf - Fatigue Striation