Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the internal side of the drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained uncleaned for a period a little longer than 1 month.
775
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Internal Surface

More from these cases

ML00135 — MIC of a Non Magnetic Drilling ToolM - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
163
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - General View
Aspect of the external side of the nominal diameter 6 3/4" drilling tool, after cleaning for inspection. Several regions of corrosion where detected where the drilling mud was adhered and remained for a period a little longer than 1 month. This tool is a high strength steel, cold worked.
125
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Localized Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion
ML00135 / May.2018
MIC of a Non Magnetic Drilling Tool
M - High Mn Austenitic SteelP - Tubular ForgingAp - O&G Well DrillingCd - Pitting Corrosion
Cm - Aspect Before AnalysisDf - Corrosion