N07718

2 cases · 5 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Secondary Cracks
Transgranular brittle aspect of the stud fracture surface.  Evidences of hydrogen embrittlement.
965
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks

More from these cases

ML00078 — Hydrogen Cracking of IN 718 Subsea ConnectorM - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Secondary Cracks
ML00075 — Hydrogen Cracking of IN 718 Subsea FastenersM - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Secondary Cracks
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks