ASTM

1 case · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ASTM — sub-branches

Quenched and tempered structure of the F22 steel forging, presenting about 230HV10 average hardness.
133
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

More from these cases

ML00178 — Cold cracks in Cr-Mo Welded ForgingM - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Tempered martensitic structure for the F22 forging base metal.
129
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite
Fusion line of the forging side, in the cap, showing the weld metal (to the top of the image) and the base metal (to the bottom of the image). The heat affected zone hardness is about 270HV10.
108
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Heat Affected Zone
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Martensite
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal

+1 more from this case →