Crevice Corrosion in a Subsea System — Aspect Before Analysis

Micrography of the pipe longitudinal base metal.
148
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Kalling Etched Micrography by OMDf - Base Metal Left Side
Transverse section of the fitting that suffered a longitudinal cracking. As polished. The wrought fitting has suffered intergranular stress corrosion cracking from the internal surface, exposed to hot caustic environment.
566
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Micrography by OMDf - Intergranular Cracking

More from these cases

ML00065 — Erosion Corrosion of Monel PipingM - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Micrographic detail of the pipe base metal presenting a granular microstructure. Some inclusions are also visible.
142
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Kalling Etched Micrography by OMDf - Base Metal Left Side
Micrography of the elbow base metal. The comparison with the pipe micrography shows an important difference of thickness.
132
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Kalling Etched Micrography by OMDf - Base Metal Right Side
Elbow base metal micrographic detail presenting a granular microstructure. Like the pipe, the microstructure reveals inclusions.
106
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Kalling Etched Micrography by OMDf - Base Metal Right Side
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Kalling Etched Micrography by OMDf - Fusion Line Left Side
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Kalling Etched Micrography by OMDf - Fusion Line Left Side

+11 more from this case →

ML00011 — Intergranular SCC of Pure NickelM - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Microstructure of the fitting in the transverse section, presenting a granular Ni austenitic structure.  No evidences of any phase in the grain boundaries.
114
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Kalling Etched Micrography by OMDf - Austenite
Microstructure of the fitting in the transverse section, presenting a granular Ni austenitic structure.  No evidences of any phase in the grain boundaries.
110
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Kalling Etched Micrography by OMDf - Austenite
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Kalling Etched Micrography by OMDf - Austenite
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Micrography by OMDf - Intergranular Cracking
ML00011 / Oct.2017
Intergranular SCC of Pure Nickel
M - Unalloyed NickelP - Wrought FittingAp - Chemical IndustryCd - Stress Corrosion
Cm - Micrography by OMDf - Corrosion Cracking