In Field Weld

2 cases · 24 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Image of the magnetic particle test, using a white contrast, presenting the cracks at the surface of the weld metal.  The cracks are transverse to the weld and do not propagate into the base metals. A forged T in the right side of the figure and a thick wall tube in the left side of the figure, both in P12 CrMo steel.
1044
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Aspect by NDTDf - Cracks
The internal surface of the 2 1/2" thickness plate drum was welded to attach a baffle plate (1/4" thick) using two fillets (one in each side of the plate to shell), but the welding procedure was not suitable since cracks appeared underbead, although they were detected only after 6 month in operation, when the baffle was removed. The picture shows a macrography of the surface, with the cracking.
698
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - NItal Etched MacroDf - Cracking

More from these cases

ML00071 — Reheating Cracking of a CrMo Vessel WeldM - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Aspect of the butt welded joint surface, after grinding to remove the reinforcement, polishing and macro etching.  There are multiple cracks, transverse to the weld and restricted to the weld metal.  The surface hardness are 167HB for the tube (left side), 180 HB for the Forged T (right side) and 272 HB for the weld metal, suggesting lack of a suitable PWHT.
181
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Surface AspectDf - Cracks
The morphology of the cracking in the weld metal is intergranular (in the previous austenite grain boundaries), and branched. The replication technique was adopted to define the nature of the cracks.
148
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Cracks
Detail of the weld metal intergranular and branched cracking (in the previous austenite grain boundaries). The replication technique was adopted to define the nature of the cracks.
125
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Cracks
The forged T presented a ferritic perlitic/bainitic structure at the surface, where the replica was conducted. The base material material hardness is 180 HB.
121
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Ferrite and Bainite
The thick wall tube presented a bainitic structure at the surface, where the replica was conducted. The base material material hardness is 167 HB.
109
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Bainite

+10 more from this case →

ML00008 — Cold Cracks in CMn Steel Pressure VesselM - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Micrography of a longitudinal section of the shell plate base metal, presenting a typical ferritic-perlitic microstructure.
149
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Higher magnification of the ferritic-perlitic microstructure of the shell plate in the longitudinal section.
129
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ.
123
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. The cracks are mainly located at the fusion line.
118
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. Several internal cracks at the fusion line.
101
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks