Forging

2 cases · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Microscopic image by scanning electron microscope (SEM) of the ring surface that presented pites under fouling deposits.
522
ML00124 / Feb.2018
MIC of a Martensitic Valve Ring
M - Martensitic Stainless SteelP - ForgingAp - EnergyCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Pitting
External surface aspect of the flange showing preferential dissolution, responsible for nucleation of the through wall cracking.
245
ML00002 / Jan.2018
Preferential Dissolution and Cracks in SDSS
M - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Cm - Surface Aspect by SEMDf - Preferential Dissolution

More from these cases

ML00124 — MIC of a Martensitic Valve RingM - Martensitic Stainless SteelP - ForgingAp - EnergyCd - Brittle Behavior
ML00124 / Feb.2018
MIC of a Martensitic Valve Ring
M - Martensitic Stainless SteelP - ForgingAp - EnergyCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Pitting
ML00124 / Feb.2018
MIC of a Martensitic Valve Ring
M - Martensitic Stainless SteelP - ForgingAp - EnergyCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Pitting
ML00124 / Feb.2018
MIC of a Martensitic Valve Ring
M - Martensitic Stainless SteelP - ForgingAp - EnergyCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Pitting
ML00124 / Feb.2018
MIC of a Martensitic Valve Ring
M - Martensitic Stainless SteelP - ForgingAp - EnergyCd - Brittle Behavior
Cm - Surface Aspect by SEMDf - Pitting
ML00002 — Preferential Dissolution and Cracks in SDSSM - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Detail of the region at the flange external surface where the material is suffering the preferential corrosion.
177
ML00002 / Jan.2018
Preferential Dissolution and Cracks in SDSS
M - Super Duplex Stainless SteelP - Fabrication WeldAp - PipingCd - Preferential Dissolution
Cm - Surface Aspect by SEMDf - Preferential Dissolution