Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
Transgranular brittle aspect of the stud fracture surface.  Evidences of hydrogen embrittlement.
965
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks

More from these cases

ML00136 — Hydrogen Cracks of Subsea StudsM - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Secondary Cracks
ML00136 / Jun.2018
Hydrogen Cracks of Subsea Studs
M - Low Alloy Medium Carbon QTP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Nital Etched Micrography by SEMDf - Cracks
ML00075 — Hydrogen Cracking of IN 718 Subsea FastenersM - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement