Ferritic Bainitic
3 cases · 25 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Intergranular Cracking

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
More from these cases

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Left Side

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks