Ferritic Bainitic

4 cases · 31 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracking
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Intergranular Cracking
Micrography of a longitudinal section of the shell plate base metal, presenting a typical ferritic-perlitic microstructure.
149
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Banded Structure

More from these cases

ML00072 — Liquation Cracks in a High Strength JointM - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Fusion Line
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Microcracks
ML00072 / Jan.2018
Liquation Cracks in a High Strength Joint
M - Low Alloy Medium Carbon QTP - Longitudinal Seam Welded PipeAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal Left Side

+7 more from this case →

ML00071 — Reheating Cracking of a CrMo Vessel WeldM - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00008 — Cold Cracks in CMn Steel Pressure VesselM - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Higher magnification of the ferritic-perlitic microstructure of the shell plate in the longitudinal section.
129
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ.
123
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. The cracks are mainly located at the fusion line.
118
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
Cold cracking of the fillet weld adopted to attach a flat support into a vessel shell in the internal side, using an unsuitable welding procedure that created a too high hardness HAZ. Several internal cracks at the fusion line.
101
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks
ML00008 / Nov.2017
Cold Cracks in CMn Steel Pressure Vessel
M - CMn SteelP - In Field WeldAp - BoilerCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Cracks

+1 more from this case →

ML00013 — Welding Cracks in Mooring ChainM - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Segregated Regions
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Non Metallic Inclusions