Ferrous Alloys
1 case · 9 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis
Condition: Welding Defect ×Microstructure: Columnar Grains ×Capture method: Scanning Electron Microscope ×clear all
Ferrous Alloys — sub-branches

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Fusion Line
More from these cases

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Heat Affected Zone

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Cracking

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Intergranular Cracking

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Cold cracking

ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by SEMDf - Intergranular Cracking