Precipitation Hardened Stainless Steel
4 cases · 20 images
Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - At the Surface

ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking

ML00076 / Jun.2017
Hydrogen Cracking of a 17-7 PH Subsea Spring
M - Precipitation Hardened Stainless SteelP - WireAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
More from these cases

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Cleavage Facets

ML00139 / Jun.2018
Hydrogen Fracture of a 17-4 PH Allen Bolt
M - Precipitation Hardened Stainless SteelP - Allen BoltAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Cleavage Facets

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Fracture

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture

ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture

ML00074 / Jun.2018
Hydrogen Cracking of a 17-4 PH Subsea Bolt
M - Precipitation Hardened Stainless SteelP - FastenerAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Ductile Fracture

ML00076 / Jun.2017
Hydrogen Cracking of a 17-7 PH Subsea Spring
M - Precipitation Hardened Stainless SteelP - WireAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture

ML00076 / Jun.2017
Hydrogen Cracking of a 17-7 PH Subsea Spring
M - Precipitation Hardened Stainless SteelP - WireAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture