Bainite

8 cases · 12 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Bainite
ML00133 / May.2018
Seam Welded Pipe Cladded with Alloy 625
M - LAS / Ni AlloyP - Longitudinal Seam Welded PipeAp - Oil and GasCd - Welding
Cm - Nital Etched Micrography by OMDf - Bainite
ML00132 / May.2018
Seamless Pipe Overlaid with Alloy 625
M - LAS / Ni AlloyP - Seamless PipeAp - Oil and GasCd - Welding
Cm - Nital Etched Micrography by OMDf - Bainite
ML00109 / Jan.2018
Thermal Spray and Fuse Layer in Forged Pin
M - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Thermal spray
Cm - Nital Etched Micrography by OMDf - Bainite
Micrography of the longitudinal section of the tube, close to the internal surface. 
A thick scale is evident, but no microstructural changes compared to the center of the tube.
183
ML00107 / Dec.2017
Carburized 9Cr1MoV Superheater Tube
M - Heat Resistant SteelP - Seamless tubeAp - BoilerCd - Carburization
Cm - Nital Etched Micrography by OMDf - Bainite
ML00081 / Aug.2017
Hydrogen Cracking of a Chromium Plated Carburized Pin
M - Low Alloy for Thermochemical TreatmentP - Chromium PlatedAp - AutomotiveCd - Hydrogen Embrittlement
Cm - Nital Etched Micrography by OMDf - Bainite
The thick wall tube presented a bainitic structure at the surface, where the replica was conducted. The base material material hardness is 167 HB.
108
ML00071 / Jan.2019
Reheating Cracking of a CrMo Vessel Weld
M - CrMo SteelP - In Field WeldAp - EnergyCd - Welding Defect
Cm - Nital etched, OMDf - Bainite
ML00013 / Apr.2017
Welding Cracks in Mooring Chain
M - Low Alloy Low Carbon QTP - Welded PartAp - OffshoreCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Bainite

More from these cases

ML00109 — Thermal Spray and Fuse Layer in Forged PinM - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Thermal spray
ML00109 / Jan.2018
Thermal Spray and Fuse Layer in Forged Pin
M - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Thermal spray
Cm - Nital Etched Micrography by OMDf - Bainite
ML00107 — Carburized 9Cr1MoV Superheater TubeM - Heat Resistant SteelP - Seamless tubeAp - BoilerCd - Carburization
Micrography of a longitudinal section of the tube in the center of the thickness, showing a ferritic-bainitic structure of this CrMoV steel.
156
ML00107 / Dec.2017
Carburized 9Cr1MoV Superheater Tube
M - Heat Resistant SteelP - Seamless tubeAp - BoilerCd - Carburization
Cm - Nital Etched Micrography by OMDf - Bainite
Micrography of a longitudinal section of the tube in the center of the thickness, showing a ferritic-bainitic structure of this CrMoV steel.
137
ML00107 / Dec.2017
Carburized 9Cr1MoV Superheater Tube
M - Heat Resistant SteelP - Seamless tubeAp - BoilerCd - Carburization
Cm - Nital Etched Micrography by OMDf - Bainite
Micrography of a longitudinal section of the tube in the center of the thickness, showing a ferritic-bainitic structure of this CrMoV steel.
142
ML00107 / Dec.2017
Carburized 9Cr1MoV Superheater Tube
M - Heat Resistant SteelP - Seamless tubeAp - BoilerCd - Carburization
Cm - Nital Etched Micrography by OMDf - Bainite