Leakage

2 cases · 8 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00180 / Mar.2022
Local Melting of Copper Cooling Tubes
M - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
Cm - Longitudinal Section AspectDf - Leakage
Region of the leakage close to the welded joint between the pipe and the 90° elbow, in the 1 1/2" nominal diameter piping, SCH 40 (3.7 mm thick). See the schematic drawing in the next figure
966
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Aspect Before AnalysisDf - Leakage

More from these cases

ML00180 — Local Melting of Copper Cooling TubesM - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
ML00180 / Mar.2022
Local Melting of Copper Cooling Tubes
M - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
Cm - Transverse Section AspectDf - Leakage
ML00180 / Mar.2022
Local Melting of Copper Cooling Tubes
M - Pure CopperP - Cooling TubeAp - SiderurgyCd - Overheating
Cm - Transverse Section AspectDf - Leakage
ML00065 — Erosion Corrosion of Monel PipingM - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Schematic drawing presenting the External piping surface
339
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Identification drawingDf - Leakage
Aspect of the piping cut in the longitudinal direction, presenting the leakage region close to the welded joint between the pipe and the 90° elbow. The original SCH 40 (3.7 mm thickness) presents an actual average thickness of 2 mm all through the piping extension, evidencing a general thinning. See the schematic drawing in the next figure.
364
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Aspect Before AnalysisDf - Leakage
Schematic drawing presenting the internal piping surface
234
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Identification drawingDf - Leakage
Detail of the internal piping surface, showing lack of deposits and a shinning surface, suggesting erosive conditions.
226
ML00065 / May.2017
Erosion Corrosion of Monel Piping
M - NiCu AlloyP - Seamless PipeAp - Chemical IndustryCd - Erosion Corrosion
Cm - Surface AspectDf - Leakage