Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - As polished micrographyDf - Intergranular Cracking
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Intergranular Cracking
ML00042 / Apr.2017
Gas Turbine Blade IN 939, Coated
M - NiCrCo AlloyP - CastAp - Gas TurbineCd - Intergranular Cracking
Cm - H2SO4+HNO3+H3PO4 Etched MicroDf - Intergranular Cracking

More from these cases

ML00137 — Brittle Fracture of a 15-5 PH Valve SpringM - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - As polished micrographyDf - Intergranular Cracking
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Kalling Etched Micrography by OMDf - Intergranular Cracking
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Kalling Etched Micrography by OMDf - Intergranular Cracking
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Kalling Etched Micrography by OMDf - Intergranular Cracking