Welding

2 cases · 7 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Micrographic detail of a longitudinal section of a 4 mm diameter wire, presenting an aligned and highly strained pearlitic structure. Base metal.
386
ML00113 / Jan.2018
Autogenous Weld of a Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
Cm - Nital Etched Micrography by OMDf - Strain hardened pearlite
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

More from these cases

ML00113 — Autogenous Weld of a Carbon Steel WireM - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
ML00113 / Jan.2018
Autogenous Weld of a Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
Cm - Nital Etched Micrography by OMDf - Martensite
ML00113 / Jan.2018
Autogenous Weld of a Carbon Steel Wire
M - Medium Carbon SteelP - WireAp - OffshoreCd - Welding
Cm - Nital Etched Micrography by OMDf - Martensite
ML00100 — Superduplex Tubing to Forging Welded JointM - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Coarse Structure