Fabrication Defect

2 cases · 4 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Fabrication Defect — sub-branches

ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Identification drawingDf - Fracture
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Identification drawingDf - Fracture

More from these cases

ML00052 — Cold Cracks in API 5CT L80 Tube Welded to a Structural PartM - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Identification drawingDf - Welded Joint
ML00069 — Liquation Cracks in SAW of Low Carbon SteelM - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00069 / May.2017
Liquation Cracks in SAW of Low Carbon Steel
M - Low Carbon SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Identification drawingDf - Welded Joint