Optical Microscope

57 cases · 475 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Nital Etched Micrography by OMDf - Corroded Thread
Quenched and tempered structure of the F22 steel forging, presenting about 230HV10 average hardness.
133
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
Micrography of a crankshaft longitudinal section at the shaft edge, in the as polished condition, presenting nodular graphite, well distruibuted.
139
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - As polished micrographyDf - At the Surface
Micrography of the longitudinal section, in the center of the thickness of the pin, presenting an aligned ferritic-austeinitic structure.
180
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Ferrite and Austenite
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - As polished micrographyDf - Close to the Internal Surface

More from these cases

ML00184 — Dissimilar Steels in a Threaded ConnectionM - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Nital Etched Micrography by OMDf - Transverse Section
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Nital Etched Micrography by OMDf - Bainitic Ferrite
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Nital Etched Micrography by OMDf - Corroded Thread
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Nital Etched Micrography by OMDf - Corroded Thread
ML00184 / Apr.2023
Dissimilar Steels in a Threaded Connection
M - Low Carbon SteelP - ForgingAp - OffshoreCd - Localized Dissolution
Cm - Nital Etched Micrography by OMDf - Oxide Layer
ML00178 — Cold cracks in Cr-Mo Welded ForgingM - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Tempered martensitic structure for the F22 forging base metal.
129
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite
Fusion line of the forging side, in the cap, showing the weld metal (to the top of the image) and the base metal (to the bottom of the image). The heat affected zone hardness is about 270HV10.
108
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Heat Affected Zone
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Martensite
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Tempered Martensite
ML00178 / Jan.2022
Cold cracks in Cr-Mo Welded Forging
M - CrMo SteelP - ForgingAp - O&G Well DrillingCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Weld Metal

+1 more from this case →

ML00177 — Cr-Mo Seam Welded TubeM - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Granular structure
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Grain refined structure
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Last Bead HAZ
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Last Bead HAZ
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Bainitic HAZ

+18 more from this case →

ML00164 — Austenitic SS Casting for Valve BodyM - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00154 — High Strength Cast Iron CrankshaftM - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
As polished micrography of the crankshaft at the shaft edge, close to the surface.  Graphite in nodules.
126
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - As polished micrographyDf - Graphite in Nodules
As polished micrographic detail of the graphite in nodules, close to the surface of the shaft edge, in a longitudinal section.
114
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - As polished micrographyDf - Graphite in Nodules
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - Nital Etched Micrography by OMDf - At the Surface
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - Nital Etched Micrography by OMDf - Matrix of ferrite and pearlite
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - Nital Etched Micrography by OMDf - Matrix of ferrite and pearlite

+12 more from this case →

ML00146 — Plastic Deformation of a SDSS Riser PinM - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Micrography of a longitudinal section, at the surface of the pin, where the thermal spray layer is sound. The thickness of the layer is about 0.3 mm.
168
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Coating Layer
Micrographic detail of a longitudinal section of the pin, at the surface, evidencing the thermal spray layer, about 0.3 mm.  The layer presents typical characteristics of multiple layers, low amount of entrapped oxides and pores.  The interface presents a high roughness level for a good adherence and some entrapped oxides. The structure of the SDSS substrate did not show thermal effects.
154
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Coating Layer
Micrography of a longitudinal section, at the damage surface of the pin, where the thermal spray layer was partially detached and broken.  The through layer breaking is ductile, typical of an overloading condition caused by the localized bending of the pin.
109
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Layer Detachment
Micrographic detail of the damage surface layer, detached and broken.  The substrate is not affected and the rupture of the layer is typically by overloading.
117
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Layer Detachment
ML00143 — Impact of a .308 Winchester on A36 PlateM - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - Nital Etched Micrography by OMDf - Ferrite and Pearlite
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - As polished micrographyDf - Transverse Section
ML00143 / Aug.2018
Impact of a .308 Winchester on A36 Plate
M - Low Carbon SteelP - Rolled PlateAp - StructureCd - Pierced
Cm - As polished micrographyDf - Melted film

+22 more from this case →

ML00141 — Brittle Fracture of a Corroded Gray Cast IronM - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - As polished micrographyDf - In the Center of the Thickness
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - As polished micrographyDf - Close to the External Surface
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Close to the Internal Surface
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Graphite in Flakes
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Nital Etched Micrography by OMDf - Predominantly Pearlitic

+19 more from this case →