Optical Microscope

4 cases · 8 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Optical Microscope — sub-branches

ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal
Micrography of the pipe base metal, in a longitudinal section, presenting a slight banding and a refined structure.
147
ML00153 / Jan.2019
X52 in a Tubular Structure
M - CMn SteelP - Seamless PipeAp - StructureCd - Qualified
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00110 / Jan.2018
Non Conformance in Spray and Fuse Pin
M - Low Alloy Medium Carbon QTP - Tubular ForgingAp - O&G Well DrillingCd - Heat Treatment Defect
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal

More from these cases

ML00177 — Cr-Mo Seam Welded TubeM - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00177 / Dec.2021
Cr-Mo Seam Welded Tube
M - CrMo SteelP - Longitudinally Seam WeldedAp - Fired HeaterCd - Not according to spec
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00153 — X52 in a Tubular StructureM - CMn SteelP - Seamless PipeAp - StructureCd - Qualified
Micrography of the pipe base metal, in a longitudinal section.  The ferritic structure is refined and it is possible to identify a small variation in the ferritic grain size, that is promoting the slight banding effect.
119
ML00153 / Jan.2019
X52 in a Tubular Structure
M - CMn SteelP - Seamless PipeAp - StructureCd - Qualified
Cm - Nital Etched Micrography by OMDf - Base Metal
ML00067 — Cold Cracks in C-Mn SAW Weld MetalM - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
ML00067 / May.2017
Cold Cracks in C-Mn SAW Weld Metal
M - CMn SteelP - Fabrication WeldAp - AutomotiveCd - Welding Defect
Cm - Nital Etched Micrography by OMDf - Base Metal