Crevice Corrosion in a Subsea System — Aspect Before Analysis

Optical Microscope — sub-branches

Micrography of the tubing fusion line. The welding was conducted in two passes. The average hardness at the heat affected zone of the tubing is 257 HV5.
825
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Fusion Line Left Side

More from these cases

ML00100 — Superduplex Tubing to Forging Welded JointM - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - HAZ Left Side
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - HAZ Left Side
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Base Metal Left Side
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

+10 more from this case →