Oxalic Acid Electrolytic Etch

2 cases · 13 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
Optical micrography of a longitudinal section of the fractured bolt, at the thread.  The material is austenitic, free from carbides, and the threads were almost removed by the stress corrosion cracks.
756
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks

More from these cases

ML00164 — Austenitic SS Casting for Valve BodyM - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00164 / Jun.2020
Austenitic SS Casting for Valve Body
M - Austenitic Stainless SteelP - CastingAp - ValveCd - Typical manufacturing
Cm - Oxalic Acid Electrolytic EtchDf - Delta ferrite
ML00157 — Bolts Under Chloride SCC ConditionsM - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Low magnification micrography, by optical microscope, of the longitudinal section of a damaged bolt, in the center of the thickness. The microstructure is austenitic, free from carbides.
100
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Austenite
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Strain Hardened
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks
ML00157 / Feb.2020
Bolts Under Chloride SCC Conditions
M - Austenitic Stainless SteelP - BoltAp - Oil and GasCd - Stress Corrosion
Cm - Oxalic Acid Electrolytic EtchDf - Stress Corrosion Cracks

+1 more from this case →