NaOH Electrolytic Etched Micro

2 cases · 21 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Micrography of the longitudinal section, in the center of the thickness of the pin, presenting an aligned ferritic-austeinitic structure.
180
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Ferrite and Austenite
Micrography of the tubing fusion line. The welding was conducted in two passes. The average hardness at the heat affected zone of the tubing is 257 HV5.
825
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Fusion Line Left Side

More from these cases

ML00146 — Plastic Deformation of a SDSS Riser PinM - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Micrography of a longitudinal section, at the surface of the pin, where the thermal spray layer is sound. The thickness of the layer is about 0.3 mm.
168
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Coating Layer
Micrographic detail of a longitudinal section of the pin, at the surface, evidencing the thermal spray layer, about 0.3 mm.  The layer presents typical characteristics of multiple layers, low amount of entrapped oxides and pores.  The interface presents a high roughness level for a good adherence and some entrapped oxides. The structure of the SDSS substrate did not show thermal effects.
154
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Coating Layer
Micrography of a longitudinal section, at the damage surface of the pin, where the thermal spray layer was partially detached and broken.  The through layer breaking is ductile, typical of an overloading condition caused by the localized bending of the pin.
109
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Layer Detachment
Micrographic detail of the damage surface layer, detached and broken.  The substrate is not affected and the rupture of the layer is typically by overloading.
117
ML00146 / Jul.2018
Plastic Deformation of a SDSS Riser Pin
M - Super Duplex Stainless SteelP - PinAp - O&G Well DrillingCd - Bending
Cm - NaOH Electrolytic Etched MicroDf - Layer Detachment
ML00100 — Superduplex Tubing to Forging Welded JointM - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - HAZ Left Side
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - HAZ Left Side
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Base Metal Left Side
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure
ML00100 / Nov.2017
Superduplex Tubing to Forging Welded Joint
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Welding
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure

+10 more from this case →