Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00181 / Apr.2022
Wear of a Carburized Hypoid Gear
M - Low Alloy for Thermochemical TreatmentP - Pinion-crown assemblyAp - ShipCd - Wear
Cm - Fractography by SEMDf - Fatigue Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00009 / Sep.2017
Hydrogen Cracking of a 5" Drill Pipe S135
M - Low Alloy Medium Carbon QTP - Drill PipeAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking
More from these cases

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Broken Testpiece

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Broken Testpiece

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Intergranular Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00080 / Sep.2017
MIC of Stacking Disc Springs
M - Low Alloy Medium Carbon QTP - SpringAp - SubseaCd - Brittle Behavior
Cm - Fractography by SEMDf - Transgranular Fracture

ML00009 / Sep.2017
Hydrogen Cracking of a 5" Drill Pipe S135
M - Low Alloy Medium Carbon QTP - Drill PipeAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking

ML00009 / Sep.2017
Hydrogen Cracking of a 5" Drill Pipe S135
M - Low Alloy Medium Carbon QTP - Drill PipeAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Transgranular Cracking

ML00009 / Sep.2017
Hydrogen Cracking of a 5" Drill Pipe S135
M - Low Alloy Medium Carbon QTP - Drill PipeAp - SubseaCd - Hydrogen Embrittlement
Cm - Fractography by SEMDf - Transgranular Crack