Fractography by SEM

7 cases · 23 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fractography by SEMDf - Corrosion
ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Brittle Fracture
ML00134 / Aug.2020
Brittle Fracture of a Superduplex Valve Body
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets
The hose connector fracture surface presented different fracture micromechanisms associated to the microstructure: inclusion decohesion, small regions of intergranular fractures (probably due to cementite at grain boundaries), and cleavage of the ferritic structure.  All these mechanisms are brittle.
560
ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Brittle Fracture
Detail of the pin fracture surface, presenting both a flat aspect and a rough aspect in a shearing section of 2.5 mm width.
727
ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Fracture
The fracture surface is flat, shows the graphite nodules and cleavage of the ferritic microstructure, indicating that the material have exceeded the capacity to acomodate the stress.
945
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets

More from these cases

ML00182 — Brittle Fracture of a LAS Fixing RodM - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture
ML00182 / Jul.2022
Brittle Fracture of a LAS Fixing Rod
M - Low Alloy Medium Carbon QTP - StemAp - Mechanical IndustryCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture
ML00141 — Brittle Fracture of a Corroded Gray Cast IronM - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
ML00141 / Jul.2018
Brittle Fracture of a Corroded Gray Cast Iron
M - Gray Cast ironP - CastingAp - EngineCd - Brittle Fracture
Cm - Fractography by SEMDf - Brittle Fracture
ML00138 — Liquid Metal Embrittlement of a HSLA SteelM - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Fracture
ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture
ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Intergranular Cracking
ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Intergranular Fracture
ML00138 / Jun.2018
Liquid Metal Embrittlement of a HSLA Steel
M - High Strength Low AlloyP - Coated ProductAp - Mechanical IndustryCd - Liquid Metal Embrittlement
Cm - Fractography by SEMDf - Dimples
ML00134 — Brittle Fracture of a Superduplex Valve BodyM - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Fracture
ML00134 / Aug.2020
Brittle Fracture of a Superduplex Valve Body
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets
ML00134 / Aug.2020
Brittle Fracture of a Superduplex Valve Body
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Fracture
Cm - Fractography by SEMDf - Secondary Cracks
ML00103 — Brittle Fracture of a Free-Cutting ConnectorM - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets
ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Brittle Fracture
ML00103 / Nov.2017
Brittle Fracture of a Free-Cutting Connector
M - Low Carbon SteelP - Machined PartAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Intergranular Fracture
ML00046 — Brittle Fracture of SS Shear PinM - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Fracture appearance in a sheared region, presenting a ductile morphology for the fracture micromechanism.
109
ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Ductile Fracture
ML00046 / Jan.2018
Brittle Fracture of SS Shear Pin
M - Martensitic Stainless SteelP - Machined PartAp - EnergyCd - Intergranular Cracking
Cm - Fractography by SEMDf - Intergranular Cracking
ML00040 — Brittle Fracture of a Valve StemM - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Detail of the cleavage micromechanism.
195
ML00040 / Apr.2017
Brittle Fracture of a Valve Stem
M - Nodular Cast IronP - Valve StemAp - ShipCd - Brittle Fracture
Cm - Fractography by SEMDf - Cleavage Facets