Crevice Corrosion in a Subsea System — Aspect Before Analysis

General view of the nodular cast iron crankshaft, 240 mm long, in process of heat treatment.  The main and rod bearings, 54 mm diameter, are heat treated  by localized quenching and tempering.
1018
ML00154 / Jan.2019
High Strength Cast Iron Crankshaft
M - Nodular Cast IronP - CastingAp - EngineCd - Surface treatment
Cm - Aspect Before AnalysisDf - General View
Macroscopic aspect of the 1" shaft fracture surface, revealing beach marks at the surface typical of fatigue, initiated from the surface of the spline shaft at the gear position.
498
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Aspect Before AnalysisDf - Fatigue Fracture

More from these cases

ML00041 — Fatigue Fracture of Inconel 718 Spline ShaftM - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
xx
117
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Aspect Before AnalysisDf - At the Surface
Macroscopic aspect of the 1" shaft fracture surface, revealing beach marks at the surface typical of fatigue, initiated from the surface of the spline shaft at the gear position.
121
ML00041 / Jun.2017
Fatigue Fracture of Inconel 718 Spline Shaft
M - NiCrFe AlloyP - ShaftAp - Oil and GasCd - Vibration Induced Fatigue
Cm - Aspect Before AnalysisDf - Fatigue Fracture