Subsea

2 cases · 13 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Austenite

More from these cases

ML00094 — MIC of a Subsea Hydraulic LineM - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - NaOH Electrolytic Etched MicroDf - Coarse Structure
ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - NaOH Electrolytic Etched MicroDf - Duplex structure
ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - NaOH Electrolytic Etched MicroDf - Grain refined structure
ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - NaOH Electrolytic Etched MicroDf - Transverse Section
ML00094 / Sep.2017
MIC of a Subsea Hydraulic Line
M - Super Duplex Stainless SteelP - Fabrication WeldAp - SubseaCd - Brittle Behavior
Cm - NaOH Electrolytic Etched MicroDf - Through Wall Cracking

+1 more from this case →

ML00075 — Hydrogen Cracking of IN 718 Subsea FastenersM - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Austenite
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Fracture
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Intergranular Cracking
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Secondary Cracks
ML00075 / Jun.2018
Hydrogen Cracking of IN 718 Subsea Fasteners
M - NiCrFe AlloyP - StudAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Brittle Cracks