Oil and Gas

2 cases · 5 images

Crevice Corrosion in a Subsea System — Aspect Before Analysis

Aspect of the fracture of the spring.  Close to the surface the fracture presents the aspect of rusted spots.
132
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - Fracture
ML00078 / Jun.2017
Hydrogen Cracking of IN 718 Subsea Connector
M - NiCrFe AlloyP - ForgingAp - SubseaCd - Hydrogen Embrittlement
Cm - Kalling Etched Micrography by OMDf - Fracture

More from these cases

ML00137 — Brittle Fracture of a 15-5 PH Valve SpringM - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Fracture
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Fractography by SEMDf - Fracture
ML00137 / Mar.2021
Brittle Fracture of a 15-5 PH Valve Spring
M - Precipitation Hardened Stainless SteelP - SpringAp - Oil and GasCd - Brittle Behavior
Cm - Aspect Before AnalysisDf - Fracture