Crevice Corrosion in a Subsea System — Aspect Before Analysis

Scanning electron microscopy image of the chromium plated cylinder surface, presenting deposits and localized dissolution under deposits. There are different stages of corrosion in this region, observed in low magnification. Small areas of attack and a shallow pitting with deposits that were analyzed by EDS and revealed the presence of S.
903
ML00128 / Apr.2018
MIC of a Stored Hydraulic Cylinder
M - Low Carbon SteelP - Chromium PlatedAp - OffshoreCd - Localized Dissolution
Cm - Surface Aspect by SEMDf - Localized Corrosion
ML00052 / Apr.2017
Cold Cracks in API 5CT L80 Tube Welded to a Structural Part
M - Low Alloy SteelP - Seamless tubeAp - OffshoreCd - Welding Defect
Cm - Surface Aspect by SEMDf - Heat Affected Zone

More from these cases

ML00128 — MIC of a Stored Hydraulic CylinderM - Low Carbon SteelP - Chromium PlatedAp - OffshoreCd - Localized Dissolution
ML00128 / Apr.2018
MIC of a Stored Hydraulic Cylinder
M - Low Carbon SteelP - Chromium PlatedAp - OffshoreCd - Localized Dissolution
Cm - Surface Aspect by SEMDf - At the Surface
ML00128 / Apr.2018
MIC of a Stored Hydraulic Cylinder
M - Low Carbon SteelP - Chromium PlatedAp - OffshoreCd - Localized Dissolution
Cm - Surface Aspect by SEMDf - Corrosion
ML00128 / Apr.2018
MIC of a Stored Hydraulic Cylinder
M - Low Carbon SteelP - Chromium PlatedAp - OffshoreCd - Localized Dissolution
Cm - Surface Aspect by SEMDf - Corrosion